SA-333 vs SA-334: Why Low-Temperature Pipe and Tube Are Different Orders

Nominal-wall low-temperature pipe and minimum-wall low-temperature tube are not the same order. A clause-by-clause comparison of grade coverage, impact temperatures, tensile values, marking and test election.

Two ASME BPVC Section II specifications carry almost the same title. SA-333/SA-333M covers seamless and welded steel pipe for low-temperature service and other applications requiring notch toughness. SA-334/SA-334M covers seamless and welded carbon and alloy-steel tubes for low-temperature service. Buyers frequently treat them as interchangeable grade lists with two different covers. They are not. The product form, the wall basis, the general-requirements document, the grade count, the impact acceptance basis and the marking rule all change when the order moves from one to the other.

This article reads both specifications clause by clause from the Section II material volume. It does not reproduce dimensions, wall thickness tables or theoretical weights; Section II is the material volume and carries none of those. Every figure below is taken from the specification text itself.

Two products, two rulebooks

The first difference is in the scope clauses, and it propagates through everything else. SA-333 clause 1.1 covers nominal (average) wall seamless and welded carbon and alloy steel pipe. SA-334 clause 1.1 covers several grades of minimum-wall-thickness seamless and welded carbon and alloy-steel tubes. Both clauses warn that some product sizes may not be available because heavier wall thicknesses have an adverse effect on low-temperature impact properties, but they reach that warning from different wall definitions.

Each specification then hands marking, certification, retest and tolerance rules to a different general-requirements document. SA-333 clause 2.1 cites A999/A999M, the general requirements for alloy and stainless steel pipe. SA-334 clause 2.1 cites A1016/A1016M, the general requirements for ferritic alloy steel, austenitic alloy steel and stainless steel tubes. Switching the product form therefore switches the entire administrative rulebook, not just the chemistry table.

AttributeSA-333/SA-333MSA-334/SA-334M
Product named in clause 1.1Nominal (average) wall seamless and welded pipeMinimum-wall-thickness seamless and welded tubes
Service named in clause 1.1Low temperatures and other applications requiring notch toughnessLow temperatures
General-requirements document (clause 2.1)A999/A999MA1016/A1016M
Grades in the chemistry table (Table 1)9: Grades 1, 3, 4, 6, 7, 8, 9, 10, 117: Grades 1, 3, 6, 7, 8, 9, 11
Optional supplementary requirementProvided; applies only when specified by the purchaserS1 (nonstandard test specimens), applies only when specified (clause 1.2)
Impact-test clauseClause 14.1, temperatures from Table 4Clause 12.1, temperatures from Table 6
Hydrostatic / NDT electionClause 15.1Clause 16.1
Product marking clauseClause 16.1Clause 17.1
Unit-system clauseClause 1.2Clause 1.3

Both unit-system clauses say the same thing in slightly different words: inch-pound and SI values are to be regarded separately as standard, they may not be exact equivalents, and combining values from the two systems may result in non-conformance. The inch-pound units apply unless the “M” designation is specified in the order. That single line is why a metric conversion copied from a catalogue is not a substitute for the printed table.

Grade coverage and minimum impact test temperature

Grades 4 and 10 exist in SA-333 and do not exist in SA-334. More importantly, Grade 11 exists in both but is treated completely differently. The table below joins SA-333 Table 4 and SA-334 Table 6. A dash means the grade has no row in that specification’s impact temperature table.

GradeIn SA-333 Table 1In SA-334 Table 1SA-333 Table 4, min impact test tempSA-334 Table 6, impact test temp
Grade 1YesYes−50 °F / −45 °C−50 °F / −45 °C
Grade 3YesYes−150 °F / −100 °C−150 °F / −100 °C
Grade 4YesNo−150 °F / −100 °C—
Grade 6YesYes−50 °F / −45 °C−50 °F / −45 °C
Grade 7YesYes−100 °F / −75 °C−100 °F / −75 °C
Grade 8YesYes−320 °F / −195 °C−320 °F / −195 °C
Grade 9YesYes−100 °F / −75 °C−100 °F / −75 °C
Grade 10YesNo−75 °F / −60 °C—
Grade 11YesYes−320 °F / −195 °C— (clause 12.1: impact test not required)

For the six grades that appear in both impact tables, the temperatures agree. That agreement is exactly what makes the two exceptions dangerous. SA-334 clause 12.1 states plainly that the impact test is not required for Grade 11, and Table 6 has no Grade 11 row. SA-333 Table 4 does have a Grade 11 row, at −320 °F / −195 °C, and SA-333 clause 14.1 requires that material furnished and marked to the specification be impact tested at the Table 4 temperature for its grade. An order that says only “low-temperature Grade 11” therefore produces a tested product under one specification and an untested one under the other.

Grade 8 is a second, subtler trap. SA-334 clause 12.2 does not use absorbed energy for Grade 8: each notched-bar impact specimen must display lateral expansion opposite the notch of not less than 0.015 in. (0.38 mm), with a defined retest path in clause 12.2.1 when one specimen falls between 0.010 and 0.015 in. SA-334 Table 5 sets minimum average absorbed-energy values for Grades 1, 3, 6, 7 and 9 only, on a specimen-size scale from 10 by 10 mm down to 10 by 2.5 mm. So even inside SA-334, the acceptance basis is not uniform across the grade list.

Tensile requirements under SA-334

The chemistry tables also differ in width. SA-333 Table 1 prints nine grade columns and includes nickel, chromium, copper, aluminium, vanadium, columbium, molybdenum and cobalt rows for various grades. SA-334 Table 1 prints seven grade columns; its chromium, cobalt and molybdenum rows carry a limit only for Grade 11 (0.50 max each), and its copper row carries 0.75–1.25 % for Grade 9. Grade 8 nickel is 8.40–9.60 % and Grade 11 nickel is 35.0–37.0 % in both tables, so the two high-nickel grades are not chemically different between the specifications. The difference is in which grades exist and which test regime each one sits under.

SA-334 Table 3 gives the following minimum tensile and yield values. These are SA-334 values only; a purchaser must not carry them across to an SA-333 order.

SA-334 gradeTensile strength, min (ksi)Tensile strength, min (MPa)Yield strength, min (ksi)Yield strength, min (MPa)
Grade 15538030205
Grade 36545035240
Grade 66041535240
Grade 76545035240
Grade 810069075520
Grade 96343546315
Grade 116545035240

Marking, specimen size and who chooses the test

Both specifications require an “LT” marking followed by the impact test temperature, and both restrict it in the same way. SA-333 clause 16.1 requires the marking to state whether the pipe is hot finished, cold drawn, seamless or welded, plus the schedule number and “LT” with the test temperature; SA-334 clause 17.1 requires the marking to state hot-finished, cold-drawn, seamless or welded, plus “LT” with the test temperature. Where a lower test temperature was required because of reduced specimen size, both clauses say the higher temperature applicable to a full-size specimen should be marked instead.

Clause 16.1.1 in SA-333 and clause 17.1.1 in SA-334 then add the same condition: when the finished size is too small to obtain subsize impact specimens, the “LT” temperature must not be marked unless supplementary requirement S1 is specified. SA-334 S1.1 says that in that situation testing becomes a matter of agreement between manufacturer and purchaser. This is a genuine procurement decision, not a formality. A small-diameter tube ordered without S1 will not carry a test temperature in its marking, and the buyer who assumed it would has no way to reconstruct the test condition from the stencil.

The hydrostatic versus nondestructive electric test election is also identical in shape. SA-333 clause 15.1 says each pipe shall be subjected to one or the other and that the type of test is at the manufacturer’s option unless otherwise specified in the purchase order; SA-334 clause 16.1 says the same for each tube under A1016/A1016M. Both point back at their own general-requirements document for the test method. A comparison of the two verification methods explains what each can and cannot detect, and a five-rule hydrostatic test comparison sets out how the pressure basis differs between the steel and nickel-alloy rulebooks.

What to put on the order

Name the specification including the M designation if SI units are to govern. Name the product form and the wall basis explicitly, because “pipe” and “tube” are not interchangeable here. State the grade, then check that the grade actually exists in the chosen specification: Grade 4 and Grade 10 cannot be ordered to SA-334. State the impact test temperature and, for SA-334 Grade 8, confirm that the lateral-expansion criterion is understood rather than an absorbed-energy figure. Invoke S1 if subsize specimens are impossible and an “LT” temperature is required. Specify which of the hydrostatic or nondestructive electric tests is to be performed, rather than leaving the election to the mill. Confirm the certificate and marking requirements against the applicable general-requirements document, A999/A999M or A1016/A1016M. Finally, keep the two unit systems separate in the documents you issue.

For help turning a low-temperature duty into a specification line, see the pipe purchase order checklist or reach our quotation desk with the design temperature, product form and size range. We will confirm the grade and test requirements against the named specification before quoting.

Sources. ASME BPVC Section II, SA-333/SA-333M (identical with ASTM A333/A333M-16), clauses 1.1, 1.2, 2.1, 14.1, 14.1.2, 15.1, 16.1, 16.1.1, 16.1.2, Tables 1, 4 and 6; SA-334/SA-334M (identical with ASTM A334/A334M-04a(2016)), clauses 1.1, 1.2, 1.3, 2.1, 12.1, 12.2, 12.2.1, 16.1, 17.1, 17.1.1, S1.1, Tables 1, 3, 5 and 6. All read from the local Section II specification cache.

Related products: nickel alloy seamless pipe and tube · Inconel 625 seamless pipe · Hastelloy C-276 seamless pipe · pipe and tube. Supplied to the applicable ASTM / ASME specifications with EN 10204 3.1 mill test certificates; confirm grade, size and quantity with our engineers.

Product Enquiry