Six specifications, six proof tests, one phrase
Ask a supplier for nickel alloy pipe and the answer will almost always include the words “hydrostatic test to 1 000 psi”. That phrase covers six different rules in the ASME nickel alloy pipe specifications, and the rules do not agree on the equation, on the wall thickness to use, on the diameter to use, on what the 1 000 psi figure is, or on whether the test is a floor or a ceiling. Two specifications print an equation with a correction term in the denominator and three print one without. One specification tests to a fixed fibre stress that has nothing to do with the yield strength of the alloy. One uses the average wall thickness where the others use the minimum permitted wall.
None of this is academic. A buyer who sizes the proof test from the wrong equation, or from the wrong definition of the wall thickness, specifies a test that the mill does not run and the drawing does not describe. On copper-nickel, the equation without the correction term understates the required pressure by up to 24.6 % at the small sizes.
The six rules are set out below exactly as the specifications print them. Everything in this article is quoted from ASME BPVC Section II, and the pressures are our own calculation from the printed equations and the printed dimensions, labelled as such wherever they appear. None of the supplier pages we sampled for these products carries a per-size test pressure table, so the numbers below are the only place they exist in public.
The six rules side by side
This is the table to keep next to the purchase order. Read across it for the equation, then down for the definition of each variable, because two of the four columns are where the specifications genuinely disagree with each other.
| Clause | Product form | Equation as printed | S, the allowable fibre stress | t, the wall thickness used | D, the diameter used | What the 1 000 psi figure does | Hold time |
|---|---|---|---|---|---|---|---|
| SB-829 5.2 | Seamless nickel alloy pipe and tube | P = 2St/D | Lower of 2/3 of the specified minimum 0.2 % offset yield strength or 1/4 of the specified minimum ultimate strength, for the material in the condition furnished | Minimum wall thickness permitted, including minus tolerance if any | Nominal outside diameter | 1 000 psi, provided the fibre stress does not exceed the allowable. Where 1 000 psi would exceed the allowable, the equation caps it. Above 1 000 psi by agreement (NOTE 1) | 5 s |
| SB-775 5.3.1 | Welded nickel alloy pipe | P = 2St/D | Same definition as SB-829 5.2 | Minimum wall thickness permitted, including minus tolerance if any (identical wording to SB-829 5.2) | Nominal outside diameter | 1 000 psi, with the same proviso, so the equation caps it where 1 000 psi would exceed the allowable. No NOTE permitting more | Long enough to inspect the entire welded seam |
| SB-861 16.1 | Titanium seamless pipe and tube | P = SEt/(R₀ − 0.4t), equation (2) | One half of the minimum specified yield strength at room temperature | Wall thickness | R₀ is the outside tube radius, not the diameter. E = 1.0 for seamless pipe | 16.2 caps it at 2 500 psi for sizes 3 in. and under and 2 800 psi above 3 in. | 5 s |
| SB-658 13.2 | Zirconium pipe | P = 2St/D | Three fourths of the minimum yield strength of the pipe | AVERAGE wall thickness of the pipe, not the minimum and not the nominal | Nominal diameter of the pipe | 5 000 psi [35 MPa] ceiling | Not stated |
| SB-466 11.2.2 | Copper-nickel seamless tube | P = 2St/(D − 0.8t), equation (1) | Fixed at 7 000 psi [48 MPa] fibre stress, not a fraction of the yield strength | Wall thickness of the material | Outside diameter of the material, so the measured outside diameter and not the nominal size | 11.2.2.1 no pressure gage reading over 1 000 psi [7 MPa] unless specifically stipulated in the contract or purchase order | Not stated |
| SB-467 11.3.1 | Copper-nickel welded pipe | P = 2St/(D − 0.8t), equation (1) | Fixed at 7 000 psi (48 MPa) fibre stress | Wall thickness of the pipe | Outside diameter of the pipe | The pipe need not be tested over 1 000 psig (7 MPa) unless so specified | Not stated |
Two rows in that table deserve to be read twice. The first is t in SB-829 and SB-775: there is no difference. Clause 5.2 and clause 5.3.1 print the same equation P = 2St/D, define S identically as the lower of two thirds of the specified minimum 0.2 % offset yield strength or one quarter of the specified minimum ultimate strength, and define t as the minimum wall thickness permitted, including minus tolerance, if any. Both use the nominal outside diameter for D. A buyer who assumes the seamless and welded general requirements take wall thickness from different bases will write the wrong acceptance wall into one of the two purchase orders. The differences that actually matter lie elsewhere: SB-829 5.2 NOTE 1 permits a higher test pressure by agreement while SB-775 has no equivalent note, SB-829 5.2.1 requires a 5 s hold while SB-775 5.3.1.1 requires only long enough to inspect the entire welded seam, and SB-775 5.3.2 adds a 150 psi underwater pneumatic test that SB-829 does not contain.
The second is the difference in D between SB-829 and SB-466. SB-829 uses the nominal outside diameter. SB-466 clause 11.2.2 uses the outside diameter of the material, which is the measured outside diameter on the certified pipe rather than the nominal size. For a copper-nickel tube ordered at a nominal size, the diameter that belongs in the calculation is the one on the mill certificate.
On the 1 000 psi figure itself, the two nickel alloy rules are often described as one being a flat value and the other a minimum. SB-829 clause 5.2 reads “tested by the manufacturer to an internal hydrostatic pressure of 1000 psi”, and SB-775 clause 5.3.1 reads “tested by the manufacturer to a minimum internal hydrostatic pressure of 1000 psi”. Both clauses carry the same proviso, that the fibre stress calculated from the equation does not exceed the allowable fibre stress for the material, and that proviso caps the 1 000 psi figure in both cases wherever 1 000 psi would produce a fibre stress above the allowable. The wording differs; the arithmetic does not. The difference that does change what a buyer can ask for is the NOTE. SB-829 clause 5.2 NOTE 1 permits a test at a pressure greater than 1 000 psi upon agreement between purchaser and manufacturer, provided the allowable fibre stress is not exceeded. SB-775 has no equivalent note anywhere in the volume.
Two product specifications add their own overlay on top of the general requirements. SB-622 clause 8.1, for Hastelloy C-276, permits hydrostatic testing at a pressure greater than 1 000 psi upon agreement between the purchaser and manufacturer or at the option of the manufacturer, provided the allowable fibre stress per Specification B829 is not exceeded. SB-444 clause 9.1, for Alloy 625, states the allowable fibre stress directly for that grade, 30 000 psi for Grade 1 and 25 000 psi for Grade 2, and clause 9.1.1 permits pipe or tube to be tested to one and a half times that allowable fiber stress when so agreed between the manufacturer and the purchaser.
And the difference in the copper-nickel rules themselves is worth stating plainly: SB-466 is the seamless specification and SB-467 is the welded one, and clause 3.1 of SB-466 adopts the general requirements of ASTM B251/B251M, while SB-467 has no general requirements section at all and stands on its own. A seamless copper-nickel order and a welded copper-nickel order are not governed by a common framework. The full framework difference is set out on our copper-nickel 90-10 and 70-30 seamless pipe and tube page.
The same pipe, six answers
The table below applies each rule to one common geometry: ANSI B36.19 Schedule 40S, at five nominal sizes. The dimension table is held constant on purpose, so what changes between the columns is the rule and nothing else. The allowable fibre stress used for each column is the one that rule would take for its own typical grade, and each is stated in the note under the table.
| NPS | OD, in. | Nominal wall, in. | SB-829 and SB-775, psi | SB-861 Grade 2 titanium, psi | SB-658 R60702 zirconium, psi | SB-466 copper-nickel, psi |
|---|---|---|---|---|---|---|
| 2 | 2.375 | 0.154 | 1,000 | 2,500 | 2,918 | 957 |
| 4 | 4.500 | 0.237 | 1,000 | 2,199 | 2,370 | 770 |
| 6 | 6.625 | 0.280 | 1,000 | 1,750 | 1,902 | 612 |
| 8 | 8.625 | 0.322 | 1,000 | 1,539 | 1,680 | 539 |
| 12 | 12.750 | 0.375 | 1,000 | 1,205 | 1,324 | 422 |
The notes on the stresses: the SB-829 and SB-775 columns use 25 000 psi, which is the allowable fibre stress for C-276 (UNS N10276) calculated as the lower of two thirds of the 41 ksi minimum yield strength and one quarter of the 100 ksi minimum tensile strength, per SB-829 clause 5.2. The SB-861 column uses 20 000 psi, one half of the 40 ksi minimum yield strength of titanium Grade 2 per SB-861 Table 5. The SB-658 column uses 22 500 psi, three fourths of the 30 ksi minimum yield strength of R60702 per SB-658 Table 3. The SB-466 column uses the fixed 7 000 psi [48 MPa] fibre stress that the clause itself sets.
The result is the point of this article. The same NPS 12 Schedule 40S pipe is proof tested at 1 000 psi under SB-829 and SB-775, at 1 205 psi under SB-861, at 1 324 psi under SB-658 and at 422 psi under SB-466. One geometry, five rules, five different test pressures, and the highest of them is three times the lowest. A “1 000 psi hydrostatic test” on a purchase order therefore does not identify a test. It identifies a clause.
Twelve of the thirty rows have a calculated pressure below 1 000 psi, and on those sizes the test is set by the material and geometry rather than by the gage limit. On the regular wall the calculated pressure falls below 1 000 psi from SPS 3/4 upward, and it falls away from there: 721 psi at SPS 1, 503 psi at SPS 2 and 288 psi at SPS 6. On the extra strong wall the calculated pressure stays above 1 000 psi until SPS 5, where it works out to exactly 1 000 psi, and at SPS 6 it is 975 psi. On those sizes the specification asks for a fibre stress of 7 000 psi in the material and gets it from a modest pressure, because the fixed 7 000 psi figure is a property of the alloy family rather than of the manufacturing route.
Where each ceiling stops binding
Four of the six rules put a numerical ceiling on the test pressure rather than a floor, and in each case the ceiling governs over a wide part of the size range. That is worth knowing before a buyer asks for a specific test pressure, because on those sizes the specification does not allow the higher pressure to be called for without an agreement with the mill. SB-467 carries the same kind of limit as SB-466, so the table does not repeat it.
| Clause | Grade or schedule | The limit | Where the limit stops binding |
|---|---|---|---|
| SB-658 13.2 | R60702 | 5 000 psi [35 MPa] | 5 000 psi governs until 3/4 Schedule 40S, where the calculated pressure falls below the ceiling |
| SB-658 13.2 | R60704 | 5 000 psi [35 MPa] | 5 000 psi governs until 11/4 Schedule 40S, where the calculated pressure falls below the ceiling |
| SB-658 13.2 | R60705 | 5 000 psi [35 MPa] | 5 000 psi governs until 31/2 Schedule 40S, where the calculated pressure falls below the ceiling |
| SB-861 16.2 | Grade 2, Schedule 10S | 2 500 psi up to 3 in., 2 800 psi above | The ceiling governs until NPS 1-1/2, where the calculated pressure falls below it |
| SB-861 16.2 | Grade 2, Schedule 40S | 2 500 psi up to 3 in., 2 800 psi above | The ceiling governs until NPS 3, where the calculated pressure falls below it |
| SB-861 16.2 | Grade 2, Schedule 80S | 2 500 psi up to 3 in., 2 800 psi above | The ceiling governs until NPS 6, where the calculated pressure falls below it |
| SB-466 11.2.2.1 | Regular wall | No gage reading over 1 000 psi [7 MPa] | The calculated pressure falls below 1 000 psi from SPS 3/4 upward, so on those sizes the geometry sets the test rather than the clause |
| SB-466 11.2.2.1 | Extra Strong wall | No gage reading over 1 000 psi [7 MPa] | The calculated pressure falls below 1 000 psi from SPS 6 upward, so on those sizes the geometry sets the test rather than the clause |
Two of those rows are counter-intuitive. Under SB-861 the 2 500 psi and 2 800 psi ceilings govern on every Schedule 40S and Schedule 80S wall at every size, so for the schedules a titanium buyer normally orders, the proof test is set by the clause and not by the material. Only the thin Schedule 10S walls, from NPS 6 upward, drop below the ceiling, and there the grade separates the two figures: at NPS 10 Schedule 10S, Grade 2 is tested to 622 psi and Grade 5 to 1 865 psi.
Under SB-658 the 5 000 psi ceiling governs on the small sizes, and the point at which it stops binding differs by grade, because R60705 carries 1.8 times the allowable fibre stress of R60702. At NPS 12 Schedule 40S the three grades are tested to 1 324 psi, 1 544 psi and 2 426 psi.
The copper-nickel table, and the equation that is often printed wrong
The table below is the SB-466 pressure table, worked out from the SB-466 Table X1.1 dimensions at the regular and extra strong walls. It carries two numbers because the clause deals in two. The first is the pressure that produces the 7 000 psi fibre stress that clause 11.2.2 demands, calculated from the printed equation. The second is the pressure the tube is actually tested to, because clause 11.2.2.1 says the tube “need not be subjected to a pressure gage reading over 1 000 psi [7 MPa]” unless the contract or purchase order specifically stipulates otherwise. Where the calculated pressure exceeds 1 000 psi the gage limit is what relieves the mill of driving the pressure to the calculated figure. Where the calculated pressure is itself below 1 000 psi there is no relief to apply, and the full calculated pressure is the test.
| SPS | Wall | Nominal wall, in. | OD, in. | Pressure for 7 000 psi fibre stress, psi | MPa | Pressure the tube is tested to, psi | Basis |
|---|---|---|---|---|---|---|---|
| 1/8 | Regular | 0.058 | 0.405 | 2,264 | 16 | 1,000 | Gage limited to 1 000 psi |
| 1/8 | Extra Strong | 0.100 | 0.405 | 4,308 | 30 | 1,000 | Gage limited to 1 000 psi |
| 1/4 | Regular | 0.065 | 0.540 | 1,865 | 13 | 1,000 | Gage limited to 1 000 psi |
| 1/4 | Extra Strong | 0.123 | 0.540 | 3,899 | 27 | 1,000 | Gage limited to 1 000 psi |
| 3/8 | Regular | 0.065 | 0.675 | 1,461 | 10 | 1,000 | Gage limited to 1 000 psi |
| 3/8 | Extra Strong | 0.127 | 0.675 | 3,101 | 21 | 1,000 | Gage limited to 1 000 psi |
| 1/2 | Regular | 0.065 | 0.840 | 1,155 | 8 | 1,000 | Gage limited to 1 000 psi |
| 1/2 | Extra Strong | 0.149 | 0.840 | 2,894 | 20 | 1,000 | Gage limited to 1 000 psi |
| 3/4 | Regular | 0.065 | 1.050 | 912 | 6 | 912 | Full calculated pressure |
| 3/4 | Extra Strong | 0.157 | 1.050 | 2,378 | 16 | 1,000 | Gage limited to 1 000 psi |
| 1 | Regular | 0.065 | 1.315 | 721 | 5 | 721 | Full calculated pressure |
| 1 | Extra Strong | 0.182 | 1.315 | 2,179 | 15 | 1,000 | Gage limited to 1 000 psi |
| 11/4 | Regular | 0.072 | 1.660 | 629 | 4 | 629 | Full calculated pressure |
| 11/4 | Extra Strong | 0.194 | 1.660 | 1,805 | 12 | 1,000 | Gage limited to 1 000 psi |
| 11/2 | Regular | 0.072 | 1.900 | 547 | 4 | 547 | Full calculated pressure |
| 11/2 | Extra Strong | 0.203 | 1.900 | 1,636 | 11 | 1,000 | Gage limited to 1 000 psi |
| 2 | Regular | 0.083 | 2.375 | 503 | 3 | 503 | Full calculated pressure |
| 2 | Extra Strong | 0.221 | 2.375 | 1,408 | 10 | 1,000 | Gage limited to 1 000 psi |
| 21/2 | Regular | 0.083 | 2.875 | 414 | 3 | 414 | Full calculated pressure |
| 21/2 | Extra Strong | 0.280 | 2.875 | 1,479 | 10 | 1,000 | Gage limited to 1 000 psi |
| 3 | Regular | 0.095 | 3.500 | 388 | 3 | 388 | Full calculated pressure |
| 3 | Extra Strong | 0.304 | 3.500 | 1,307 | 9 | 1,000 | Gage limited to 1 000 psi |
| 31/2 | Regular | 0.095 | 4.000 | 339 | 2 | 339 | Full calculated pressure |
| 31/2 | Extra Strong | 0.321 | 4.000 | 1,201 | 8 | 1,000 | Gage limited to 1 000 psi |
| 4 | Regular | 0.109 | 4.500 | 346 | 2 | 346 | Full calculated pressure |
| 4 | Extra Strong | 0.341 | 4.500 | 1,129 | 8 | 1,000 | Gage limited to 1 000 psi |
| 5 | Regular | 0.125 | 5.552 | 321 | 2 | 321 | Full calculated pressure |
| 5 | Extra Strong | 0.375 | 5.552 | 1,000 | 7 | 1,000 | Exactly 1 000 psi |
| 6 | Regular | 0.134 | 6.625 | 288 | 2 | 288 | Full calculated pressure |
| 6 | Extra Strong | 0.437 | 6.625 | 975 | 7 | 975 | Full calculated pressure |
Now the equation. Clause 11.2.2 prints the equation for a thin hollow cylinder under tension as P = 2St/(D − 0.8t). The cached text of the specification renders the closing parenthesis as an exclamation mark and the minus sign as the digit two, so the clause reads “P 5 2St/~D 2 0.8t!” in a plain text extraction. Read literally, that looks like the SB-829, SB-775 and SB-658 equation. It is not, and the difference is not a rounding matter. We have cross-checked the clause against three independent published copies of ASTM B466 and B467.
The table below shows what the two equations give for the same pipe. The middle column is the equation that is frequently quoted on supplier pages, and the right-hand column is the one SB-466 actually prints.
| SPS | Wall | Nominal wall, in. | P = 2St/D, psi | P = 2St/(D − 0.8t), psi | The printed equation understates by |
|---|---|---|---|---|---|
| 1/8 | Extra Strong | 0.100 | 3,457 | 4,308 | 24.6 % |
| 1/4 | Extra Strong | 0.123 | 3,189 | 3,899 | 22.3 % |
| 3/8 | Extra Strong | 0.127 | 2,634 | 3,101 | 17.7 % |
| 1/2 | Extra Strong | 0.149 | 2,483 | 2,894 | 16.5 % |
| 3/4 | Extra Strong | 0.157 | 2,093 | 2,378 | 13.6 % |
| 1/8 | Regular | 0.058 | 2,005 | 2,264 | 12.9 % |
| 1 | Extra Strong | 0.182 | 1,938 | 2,179 | 12.5 % |
| 1/4 | Regular | 0.065 | 1,685 | 1,865 | 10.7 % |
| 11/4 | Extra Strong | 0.194 | 1,636 | 1,805 | 10.3 % |
| 11/2 | Extra Strong | 0.203 | 1,496 | 1,636 | 9.3 % |
At the small sizes the difference is not marginal. On the extra strong wall at SPS 1/8 the equation without the correction term gives 3 457 psi where the specification’s equation gives 4 308 psi, a shortfall of 24.6 %. On the regular wall at SPS 1/2 it gives 2 483 psi against 2 894 psi. A buyer who takes the printed figure from the wrong equation and writes it into the purchase order as the required test pressure has specified less than SB-466 requires, and the mill will either test to the specification anyway, or accept the order and test to the lower figure. Which of those two things happens is a function of the inspection regime the order carries.
For completeness, the two forms are the same equation written two ways. SB-861 clause 16.1 prints P = SEt/(R₀ − 0.4t) with E = 1.0 for seamless pipe and R₀ the outside tube radius. Substituting R₀ = D/2 gives (R₀ − 0.4t) = (D − 0.8t)/2, so the equation becomes 2SEt/(D − 0.8t), and with E = 1.0 that is exactly 2St/(D − 0.8t). We have asserted that equivalence numerically across every dimension row of the table. SB-861 and SB-466 are therefore the same rule expressed in two notations, while SB-829, SB-775 and SB-658 use the equation without the correction term.
What to write on the order
The practical answer for a purchase order is short. Name the product specification and the clause, not just the pressure. “Hydrostatic test to 1 000 psi per ASME SB-829” and “hydrostatic test to 1 000 psi” are not the same instruction, and the second one is the more common of the two.
Where the order needs a figure that the specification’s own wording leaves to agreement, say which of the two numbers is wanted. Under SB-829 clause 5.2 NOTE 1 the test may be above 1 000 psi by agreement between purchaser and manufacturer, so long as the allowable fibre stress is not exceeded. Under SB-775 clause 5.3.1 there is no equivalent note, so on that route a higher pressure is not available by agreement at all. Under SB-861 clause 16.2 the purchaser may require one and a half times the specified working pressure for sizes 14 in. and smaller, provided the corresponding fibre stress does not exceed one half of the minimum specified yield strength, and where that figure would exceed 2 800 psi the test pressure becomes a matter of agreement between the manufacturer and the purchaser.
Two alloys carry their own overlay and are worth checking by name. SB-622 clause 8.1, governing Hastelloy C-276, permits hydrostatic testing above 1 000 psi upon agreement between the purchaser and manufacturer or at the option of the manufacturer, provided the allowable fibre stress per Specification B829 is not exceeded. SB-444 clause 9.1, governing Alloy 625, states the allowable fibre stress for that alloy outright, 30 000 psi for Grade 1 and 25 000 psi for Grade 2, and clause 9.1.1 permits the pipe or tube to be tested to one and a half times that allowable fiber stress when so agreed between the manufacturer and the purchaser. A buyer working to a 1 000 psi line on an Alloy 625 order should know that the specification offers a higher figure on request, and a buyer working to a 1 000 psi line on an SB-775 welded order should know that it does not.
And say what happens when the test fails, because the two families of specification do not agree there either. SB-829 clause 5.2.2 states that if any pipe or tube shows leaks during hydrostatic testing it shall be rejected. SB-775 clause 5.3.3 says the same for pipe showing leaks during hydrostatic or pneumatic testing. The word is “rejected” in both. The retest provisions are narrower than that word suggests, and it is worth reading them before assuming a second test is available. SB-829 clause 9.1 permits retests of the mechanical tests of a group or lot on additional material from the same group or lot, double the original number, and clause 9.2 permits reheat treatment and resubmission of material that fails the test requirements, with no more than two reheat treatments permitted. Neither clause is a permission to run the proof test again on the same length of pipe, and the practical route after a leaking length is a new length, not a retest.
For the pipe itself, our C-276 seamless pipe to SB-829 is proof tested under SB-829 and our Alloy 800 welded pipe to SB-775 under SB-775, and the Alloy 625 seamless pipe to SB-444 carries its own allowable fibre stress of 30 000 psi in Grade 1 and 25 000 psi in Grade 2 under SB-444 clause 9.1. If you want the same numbers applied to a size that is not on these pages, ask and we will work them from the same printed equations.
The grade-dependent strength values behind these pressure rules are collected in our nickel alloy seamless pipe guide.