Three stainless steel pipe specifications carry the grades buyers order every day, and they are routinely treated as interchangeable on a purchase order. They are not. One is a pipe specification with no duplex grades in it at all, one is a tubing specification whose dimensional and marking rules differ from its pipe sibling, and the two duplex-capable specifications do not agree on every number for the same UNS designation. Picking the right one before the order is placed is cheaper than discovering it at the goods-in gate.
What each specification actually covers
The first question is not the grade. It is whether you are buying pipe or tube, and whether the alloy is austenitic or duplex. Those two answers select the specification, and the specification then fixes everything else.
| Specification | Product covered | General requirements | Manufacture route | Heat treatment |
|---|---|---|---|---|
| SA-789/SA-789M | Stainless steel tubing of average wall thickness, or of minimum wall thickness if specified on the order | A1016/A1016M (§4.1) | Seamless or welded process, with no filler metal added (§5.1) | All tubes heat treated per Table 2 (§6.1) |
| SA-790/SA-790M | Seamless and straight-seam welded ferritic/austenitic steel pipe | A999/A999M (§5.1) | Seamless or automatic welding process, with no addition of filler metal in the welding operation (§6.1.1) | Table 1, heat treated unless the order states otherwise (§6.3) |
| SA-312/SA-312M | Seamless, straight-seam welded and heavily cold worked welded austenitic stainless steel pipe | A999/A999M | Seamless, straight-seam welded or heavily cold worked welded | Table 2, all pipe heat treated (§6.2) |
The consequential line in that table is the third one. SA-312/SA-312M contains no duplex grades. There is no S31803, no S32205 and no S32750 anywhere in its Table 1. Anyone who writes “2205 to SA-312” on an order has written a specification that cannot be satisfied by a duplex material, whatever the mill offers. The duplex grades live in SA-789 and SA-790, and the choice between those two is decided by product form: tube or pipe.
The same UNS number, two different chemistry windows
The overlap between the two tables is where most purchasing errors are made, because a buyer who has seen a grade listed in one table tends to assume the other table agrees.
| UNS | C max | Ni | Cr | Mo | N | Other elements | SA-789 vs SA-790 |
|---|---|---|---|---|---|---|---|
| S31803 | 0.030 | 4.5–6.5 | 21.0–23.0 | 2.5–3.5 | 0.08–0.20 | — | Identical |
| S32205 (2205) | 0.030 | 4.5–6.5 | 22.0–23.0 | 3.0–3.5 | 0.14–0.20 | — | Identical |
| S31500 | 0.030 | 4.3–5.2 / 4.2–5.2 | 18.0–19.0 | 2.50–3.00 | 0.05–0.10 | — | Nickel window differs |
| S32750 (2507) | 0.030 | 6.0–8.0 | 24.0–26.0 | 3.0–5.0 | 0.24–0.32 | Cu 0.50 | Identical |
| S32760 | 0.030 | 6.0–8.0 | 24.0–26.0 | 3.0–4.0 | 0.20–0.30 | Cu 0.50–1.00; W 0.50–1.00 | Identical |
| S32304 (2304) | 0.030 | 3.0–5.5 | 21.5–24.5 | 0.05–0.60 | 0.05–0.20 | Cu 0.05–0.60 | Identical |
S31500 is the exception, and it is a real one. The nickel range in SA-789 Table 1 starts at 4.3 %, while the same grade in SA-790 Table 2 starts at 4.2 %. Both are UNS S31500, and a material that passes one specification’s chemistry table can fail the other’s on nickel alone. If the order is written as “S31500 to SA-789”, the mill works to the tighter window; if it is written as “S31500 to SA-790”, it does not. That is a decision to make deliberately.
Where the mechanical requirements diverge
Strength requirements are where the two tables separate most visibly, because the same grade can be split by a different dimension in each specification.
| UNS | SA-790/SA-790M Table 3 | SA-789/SA-789M Table 4 |
|---|---|---|
| S31803 | 90 [620] / 65 [450] / 25 % / 290 HBW / 30 HRC | 90 [620] / 65 [450] / 25 % / 290 HBW / 30 HRC / 290 HV |
| S32205 | 95 [655] / 65 [450] / 25 % / 290 HBW / 30 HRC | 95 [655] / 70 [485] / 25 % / 290 HBW / 30 HRC / 290 HV |
| S32304 | 87 [600] / 58 [400] / 25 % — one row, no size split | OD 1 in. [25 mm] and under: 100 [690] / 65 [450] — OD above 1 in.: 87 [600] / 58 [400] |
| S32003 | Split on thickness: 100 [690] / 70 [485] to 0.187 in. [5.00 mm], then 95 [655] / 65 [450] | Split on wall: 100 [690] / 70 [485] to 0.187 in. [5.00 mm], then 95 [655] / 65 [450], with a footnote on pre-2004 values |
| S32101 | Split on thickness: 101 [700] / 77 [530] to 0.187 in. [5.00 mm], then 94 [650] / 65 [450] | Split on wall: 101 [700] / 77 [530] to 0.187 in. [5.00 mm], then 94 [650] / 65 [450] |
Two things stand out. S32304 under SA-789 carries a small-bore row at 100 [690] MPa / 65 [450] MPa that does not exist under SA-790, where the grade has one unconditional set of values: order 2304 small-bore tube to SA-789 and the mill must meet the higher strength, order the same alloy to SA-790 and it need not. And SA-789 adds a Vickers column to the hardness requirement, with a footnote that the S32003 tensile values were different before A789/A789M-04 — a reminder that a certificate written years ago may quote a value the current specification has since changed.
Two different formulas for the same super duplex grade
Both duplex specifications impose a calculated minimum, written as a footnote to the chemistry table, on the grades where pitting resistance has to be guaranteed by calculation rather than by routine analysis.
| Specification | Grade | Footnote | Requirement |
|---|---|---|---|
| SA-789 Table 1 | S32750 | C | % Cr + 3.3 × % Mo + 16 × % N ≥ 41 |
| SA-789 Table 1 | S32760 | D | % Cr + 3.3 × % Mo + 16 × % N ≥ 40 |
| SA-790 Table 2 | S32750 | D | % Cr + 3.3 × % Mo + 16 × % N ≥ 41 |
| SA-790 Table 2 | S32760 | E | % Cr + 3.3 × (% Mo + 0.5 % W) + 16 × % N ≥ 41 |
Two specifications also state the calculated minimum differently for the same super duplex grade. SA-789 §1.1 footnote D for S32760 asks for % Cr + 3.3 × % Mo + 16 × % N ≥ 40 and does not credit tungsten, even though the grade is permitted 0.50 to 1.00 % W. SA-790 §1.2 footnote E credits tungsten at half weight and raises the threshold to 41. A super duplex analysis that satisfies SA-790 automatically satisfies SA-789 for this grade; the reverse is not true.
Welding, filler metal and what the marking has to say
SA-790 also carries a filler metal table that SA-789 does not, because SA-790 permits welded pipe and therefore has to state which filler pairs with which base metal.
| Pipe UNS | Filler metal, AWS A5.9 class | Filler metal UNS |
|---|---|---|
| S31803 | ER2209 | S39209 |
| S32205 | ER2209 | S39209 |
| S31200 | ER2553 | S39553 |
| S82441 | ER2209 | S39209 |
SA-790 §15.3 restricts weld repairs to gas tungsten-arc welding with a bare filler rod of the same classification as the grade in that table; §15.3.1 allows a more highly alloyed filler only with the purchaser’s approval; §15.4 requires repaired pipe to be marked WR; and §15.5 requires the repair to be completed before heat treatment. These are conditions a buyer has to write into the purchase order to enforce afterwards.
The marking rules differ too, and both are worth checking on arrival. SA-790 §16.1 requires the manufacturer’s private identifying mark, whether the pipe is seamless or welded, and the weight for pipe larger than NPS 4 if the order asks for it. SA-789 §14.1 requires the marking to indicate whether the tubing is seamless or welded and the wall designation — average wall or minimum wall. That word tells you which dimensional basis the material was produced against.
Two acceptance points complete the picture. SA-789 §10.1 puts the choice between the nondestructive electric test and the hydrostatic test at the manufacturer’s option unless the purchase order states otherwise, so a buyer who does not name the test has not chosen one. And SA-789 §12.2 warns that the permissible outside diameter variations in Table 5 do not provide for ovality in thin-walled tubes. SA-790 §1.3 points to ANSI B36.19 for pipe dimensions.
Put simply: specify the product form first, then the grade, then the specification that matches the form and the grade, and state the tests and marking you need in the order itself. If you want duplex material, SA-312 is not an option. If you want tube, SA-789 governs, and its marking must say whether the wall was ordered on an average or minimum basis. Our pipe and tube product categories cover 2205 and 2507 in both forms, and the duplex 2205 pipe product page lists the sizes we can supply against SA-789 and SA-790.
If you want the specification confirmed against the grade on your own enquiry before you order, send the grade and the product form and we will state the governing specification, the heat treatment condition and the marking in writing. Message our sales team or use WhatsApp, and we will also confirm supply for the Hastelloy C-276 pipe listing and the rest of the nickel alloy grades we hold, with the certificate content you need for goods-in inspection.
Related products: nickel alloy seamless pipe and tube · Inconel 625 seamless pipe · Hastelloy C-276 seamless pipe · pipe and tube. Supplied to the applicable ASTM / ASME specifications with EN 10204 3.1 mill test certificates; confirm grade, size and quantity with our engineers.