Duplex 2205 Seamless Pipe is supplied by Hefei Tailan Metal to ASME SA-790, ASTM A790, with an EN 10204 3.1 mill test certificate on every lot. Our seamless and welded nickel alloy pipe range covers OD 6-610 mm and wall 0.5-40 mm. Send us your grade, size and quantity and our engineers will reply within 8 working hours.
Duplex 2205 seamless pipe is the 22 % chromium / 3 % molybdenum
nitrogen-strengthened ferritic-austenitic stainless steel supplied to
ASME SA-790 under UNS S32205. SA-790 Scope 1.1 covers
seamless and straight-seam welded ferritic/austenitic steel pipe for general
corrosive service, with particular emphasis on resistance to stress-corrosion
cracking, and warns that the steels are susceptible to embrittlement if used for
prolonged periods at elevated temperatures.
SA-790 is the correct specification for duplex pipe. The related
SA-789 is the tubing specification for the same alloys, and
SA-182 covers forged flanges and fittings. Quote the form you need.
Dual Standard Designation
| Designation | Specification | Product form |
|---|---|---|
| UNS S32205 | — | Duplex 2205 / 2205 duplex, standard grade |
| UNS S31803 | — | Earlier 2205 chemistry; looser Cr / Mo / N windows |
| ASME SA-790 | ASTM A790/A790M | Seamless and welded ferritic/austenitic pipe |
| ASME SA-789 | ASTM A789/A789M | Seamless and welded ferritic/austenitic tubing |
| ASME SA-182 | ASTM A182/A182M | Forged flanges, fittings and valves |
Chemical Composition (ASME SA-790, Table 2)
| Element, % | UNS S32205 (2205) | UNS S31803 |
|---|---|---|
| Carbon, max | 0.030 | 0.030 |
| Manganese, max | 2.00 | 2.00 |
| Phosphorus, max | 0.030 | 0.030 |
| Sulfur, max | 0.020 | 0.020 |
| Silicon, max | 1.00 | 1.00 |
| Nickel | 4.5 – 6.5 | 4.5 – 6.5 |
| Chromium | 22.0 – 23.0 | 21.0 – 23.0 |
| Molybdenum | 3.0 – 3.5 | 2.5 – 3.5 |
| Nitrogen | 0.14 – 0.20 | 0.08 – 0.20 |
SA-790 Table 2 note A: values are maxima unless a range or minimum is indicated.
Where an ellipsis appears there is no minimum and the analysis need not be determined
or reported. Copper and other elements are not required for these two grades.
Mechanical Properties (ASME SA-790, Table 3)
| Grade | Tensile, min, ksi [MPa] | Yield, min, ksi [MPa] | Elongation in 2 in. / 50 mm, min, % | Hardness, max, HBW | Hardness, max, HRC |
|---|---|---|---|---|---|
| UNS S32205 (2205) | 95 [655] | 65 [450] | 25 | 290 | 30 |
| UNS S31803 | 90 [620] | 65 [450] | 25 | 290 | 30 |
SA-790 Table 3 note A: the common name is not a trademark and is not associated
with any one producer. Yield strength is determined by the 0.2 % offset method.
Size Range
Dimensions are taken from SA-790 Appendix Table X1.1, which reproduces
the ANSI B36.19 table for welded and seamless stainless steel pipe. Outside-diameter and wall-thickness tolerances are not given in the SA-790
dimensional appendix, which contains nominal dimensions only; they are set by ASME SA-999,
and the SA-999 acceptance limits are reproduced in full further down this page.
| NPS | OD (in) | OD (mm) | Sch 5S (in / mm) | Sch 10S (in / mm) | Sch 40S (in / mm) | Sch 80S (in / mm) |
|---|---|---|---|---|---|---|
| 1/8 | 0.405 | 10.29 | — | 0.049B / 1.24 | 0.068 / 1.73 | 0.095 / 2.41 |
| 1/4 | 0.54 | 13.72 | — | 0.065B / 1.65 | 0.088 / 2.24 | 0.119 / 3.02 |
| 3/8 | 0.675 | 17.15 | — | 0.065B / 1.65 | 0.091 / 2.31 | 0.126 / 3.2 |
| 1/2 | 0.84 | 21.34 | 0.065B / 1.65 | 0.083B / 2.11 | 0.109 / 2.77 | 0.147 / 3.73 |
| 3/4 | 1.05 | 26.67 | 0.065B / 1.65 | 0.083B / 2.11 | 0.113 / 2.87 | 0.154 / 3.91 |
| 1 | 1.315 | 33.4 | 0.065B / 1.65 | 0.109B / 2.77 | 0.133 / 3.38 | 0.179 / 4.55 |
| 1 1/4 | 1.66 | 42.16 | 0.065B / 1.65 | 0.109B / 2.77 | 0.14 / 3.56 | 0.191 / 4.85 |
| 1 1/2 | 1.9 | 48.26 | 0.065B / 1.65 | 0.109B / 2.77 | 0.145 / 3.68 | 0.2 / 5.08 |
| 2 | 2.375 | 60.33 | 0.065B / 1.65 | 0.109B / 2.77 | 0.154 / 3.91 | 0.218 / 5.54 |
| 2 1/2 | 2.875 | 73.03 | 0.083 / 2.11 | 0.12B / 3.05 | 0.203 / 5.16 | 0.276 / 7.01 |
| 3 | 3.5 | 88.9 | 0.083 / 2.11 | 0.12B / 3.05 | 0.216 / 5.49 | 0.3 / 7.62 |
| 3 1/2 | 4 | 101.6 | 0.083 / 2.11 | 0.12B / 3.05 | 0.226 / 5.74 | 0.318 / 8.08 |
| 4 | 4.5 | 114.3 | 0.083 / 2.11 | 0.12B / 3.05 | 0.237 / 6.02 | 0.337 / 8.56 |
| 5 | 5.563 | 141.3 | 0.109B / 2.77 | 0.134B / 3.4 | 0.258 / 6.55 | 0.375 / 9.52 |
| 6 | 6.625 | 168.28 | 0.109 / 2.77 | 0.134B / 3.4 | 0.28 / 7.11 | 0.432 / 10.97 |
| 8 | 8.625 | 219.08 | 0.109B / 2.77 | 0.148B / 3.76 | 0.322 / 8.18 | 0.5 / 12.7 |
| 10 | 10.75 | 273.05 | 0.134B / 3.4 | 0.165B / 4.19 | 0.365 / 9.27 | 0.5B / 12.7 |
| 12 | 12.75 | 323.85 | 0.156B / 3.96 | 0.18B / 4.57 | 0.375B / 9.52 | 0.5B / 12.7 |
| 14 | 14 | 355.6 | 0.156B / 3.96 | 0.188 / 4.78 | — | — |
| 16 | 16 | 406.4 | 0.165B / 4.19 | 0.188 / 4.78 | — | — |
| 18 | 18 | 457.2 | 0.165B / 4.19 | 0.188 / 4.78 | — | — |
| 20 | 20 | 508 | 0.188B / 4.78 | 0.218B / 5.54 | — | — |
| 22 | 22 | 558.8 | 0.188B / 4.78 | 0.218B / 5.54 | — | — |
| 24 | 24 | 609.6 | 0.218B / 5.54 | 0.25 / 6.35 | — | — |
| 30 | 30 | 762 | 0.25 / 6.35 | 0.312 / 7.92 | — | — |
Standard Dimensions and Wall Thickness (ANSI B36.19 Schedule Table)
The nominal dimensions below are the published ANSI B36.19
schedule values, reproduced from ASME Section II SA-790 Appendix Table X1.1, which is
based on Table 1 of ANSI B36.19-1965. The decimal thicknesses are nominal or
average wall dimensions, which is how ASME defines them. Dimension and
thickness tolerances for the pipe itself are given by ASME SA-999, which is reproduced below.
If your order calls for tolerances tighter than the SA-999 default — for example a wall
held to a minimum rather than a nominal figure — state that on the purchase order and we
will confirm what applies to your order.
Note A — Schedules 5S and 10S wall thicknesses do not permit threading in accordance with ANSI B1.20.1.
Note B — These do not conform to ANSI B36.10.
SA-790 Table X1.1 extends to NPS 30. B Note A: Schedules 5S and 10S wall
thicknesses do not permit threading in accordance with ANSI B1.20.1. B Note B:
the marked wall thicknesses do not conform to ANSI B36.10-1979. Note 1 of Table X1.1:
the decimal thickness listed represents the nominal or average wall dimension. Send us
your NPS and wall list and we will confirm availability against mill capability.
Manufacturing Route & Heat Treatment
SA-790 6.1.1 requires the pipe to be made by the seamless process or by an automatic
welding process with no addition of filler metal in the welding operation, 6.1.2 allows
hot-finished or cold-finished at the manufacturer’s option, and 6.1.3 requires the pipe
to be pickled free of scale (where bright annealing is used, descaling is not
necessary).
SA-790 6.3 requires the pipe to be furnished in the heat-treated condition shown in
Table 1 unless the order states otherwise. For UNS S32205 the solution annealing range
is 1870 – 2010 °F (1020 – 1100 °C) with rapid cooling
in air or water. SA-790 6.3.1 allows an alternative for seamless pipe: instead of a final
furnace heat treatment, pipe may be individually quenched in water or rapidly cooled by
other means immediately after hot forming, provided the pipe is at or above the specified
minimum solution treatment temperature. SA-999 16.2 limits the deviation of metal-arc
welded pipe from a 10 ft (3.0 m) straightedge to 1/8 in. (3.2 mm), prorated for shorter
lengths.
Inspection & Certification
- Hydrostatic or electric test: SA-790 14.1 requires each pipe to be
subjected to either the nondestructive electric test or the hydrostatic test, at the
manufacturer’s option unless the purchase order states otherwise. SA-790 14.2 sets the
hydrostatic test to SA-999 22.2, except that the stress used is 50 % of the
specified minimum yield strength of the pipe — the ferritic/austenitic
stainless basis, with the test pressure calculated as P = 2St/D. - Electric test: SA-790 14.3 requires nondestructive electric testing
in accordance with Practices E213 or E309. SA-790 14.4 requires the examination for
acceptance to be performed after all mechanical processing, heat treatments and
straightening operations. - Operator qualification: SA-790 14.7 requires the test unit operator
to be certified in accordance with SNT-TC-1A or an equivalent recognised standard. - Eddy-current coil frequency: SA-790 14.8.2 limits the maximum coil
frequency to 100 kHz for specified walls up to 0.050 in., 50 kHz for walls up to
0.150 in., and 10 kHz for walls over 0.150 in. - Ultrasonic search: SA-790 14.8.3 requires a minimum nominal
transducer frequency of 2.00 MHz and a maximum nominal transducer size of 1.5 in. - Tension test: one tension test for lots of not more than 100 pipes,
specimens taken from two pipes for lots of more than 100 (SA-790 13.1). - Hardness test: Brinell or Rockwell on specimens from two pipes per
lot (SA-790 13.4). - Product analysis: SA-790 9.1 makes product analysis available at the
request of the purchaser’s inspector, with the lot size defined by NPS. - Supplementary requirements: SA-790 S1 product analysis, S2
transverse tension tests, S3 flattening test and S4 etching tests to Method E381, each
applying only when specified on the purchase order. - Certification: MTC to EN 10204 3.1 standard;
EN 10204 3.2 issued when third-party inspection is specified on the order. PMI,
corrosion testing and impact testing are available on request as supplementary
requirements.
Packing & Delivery
Plastic end caps on all sizes; steel frames or wooden crates for large diameters; VCI
anti-rust wrapping. Beveled ends standard for welding; plain ends available. Each length
is marked with the standard, grade, size, heat number and heat treatment condition
(SA-790 16.1).
Applications
Seawater and cooling water systems, desalination plant intake and product piping,
oil and gas production facilities, chemical and petrochemical process lines, pulp and
paper bleaching plant piping, flue-gas desulphurisation scrubbers, waste-heat boiler
transfer lines, and potable and industrial water treatment plant piping where chloride
attack or stress-corrosion cracking governs the material selection.
Technical Notes
1. “2205” is not one UNS number, and the two that exist are not
interchangeable. SA-790 Table 2 lists S32205 and S31803 side by side, and they
carry different windows: S32205 is nitrogen-tightened at 0.14–0.20 % with
chromium 22.0–23.0 % and molybdenum 3.0–3.5 %, while S31803 allows
chromium down to 21.0 %, molybdenum down to 2.5 % and nitrogen down to 0.08 %. Both
are sold as 2205. The trap is at the fitting end: ASME SA-182 grade F 51 is
S31803 and F 60 is S32205, with different chromium, molybdenum
and nitrogen limits and different mechanical requirements (F 51 requires 90 ksi / 620 MPa
tensile against F 60 at 95 ksi / 655 MPa). A duplex fitting made to F 51 is therefore
not the same chemistry as pipe made to S32205, even though both are called 2205. Always
write the UNS number on the order and check it on the mill certificate.
2. The hydrostatic test basis is what ties wall thickness to pressure here.
SA-790 14.2 sets the hydrostatic test at 50 % of the specified minimum yield strength
of the pipe — the ferritic/austenitic stainless basis in SA-999 22.2.1, which uses
P = 2St/D with t as the specified wall thickness and D as the specified outside
diameter. SA-999 22.2.2 caps the minimum test pressure that has to be reached at
2500 psi (17.0 MPa) for outside diameters of 3.5 in. (88.9 mm) or less and 2800 psi
(19.0 MPa) above that, and SA-999 22.2.1.1 requires the resulting pressure to be
rounded to the nearest 50 psi (0.5 MPa) below 1000 psi (7 MPa) and to the nearest
100 psi (1 MPa) at or above it. Working back from the certificate, the practical
constraint is SA-999 10.1: the minimum wall thickness at any point shall not be more
than 12.5 % under the nominal wall thickness specified. That is the number to watch
when a nominal wall is being confirmed on a thin-wall duplex line.
3. The quench is the metallurgical property, not an afterthought.
SA-790 Table 1 gives S32205 a solution annealing range of 1870–2010 °F
(1020–1100 °C) followed by rapid cooling in air or water, and 6.3.1 allows
the direct quench immediately after hot forming. Duplex stainless steel derives its
corrosion resistance from a balanced ferrite-austenite microstructure, and that
balance is set by the cooling rate out of the annealing range, because slow cooling
through the intermediate range lets sigma and chi phases precipitate and tie up
chromium and molybdenum in intermetallics at the grain boundaries instead of leaving
them in solid solution. Too slow a cool and the pitting resistance falls away; too
violent a water quench and residual stress rises. SA-790 6.1.3’s pickled surface
is part of the same picture, because a mill scale that has not been removed leaves the
surface chromium-depleted. This is also why the same alloy in a different product form
carries a different anneal window — an SA-182 F 60 forging and an SA-815
WPS32205 fitting do not use the same figures as SA-790 pipe.
Permissible Variations — the Numbers You Accept Pipe Against
Nominal dimensions are only half of a purchase order. The other half is how
far the delivered pipe is allowed to deviate from those nominal figures, and
that is where inspection disputes usually start. For duplex pipe under ASME
SA-790, the acceptance tolerances are not written inside SA-790 itself: SA-790
5.1 makes the current edition of ASME SA-999/A999M the governing
general-requirements specification unless SA-790 says otherwise, and SA-790 12.1
confirms it by pointing straight back at the SA-999 Permissible Variations in
Wall Thickness section. SA-790 departs from SA-999 only where it says so
explicitly, and on lengths it does: SA-790 11.1.2 permits a definite cut length
to be no less than the length specified and no more than 1/4 in. (6 mm) over
it, which is the same limit SA-999 13.1 sets for seamless and welded pipe.
Three acceptance limits therefore govern SA-790 duplex pipe, and all three
can be written straight into an incoming-inspection plan.
1. Outside diameter tolerance — ASME SA-999 Table 1
SA-999 12.1 gives the permissible variations in outside diameter and states
that they include ovality, except as provided in 12.2 and 12.2.1. The
following is the complete seven-row SA-999 Table 1.
| NPS size range (in) | DN range (mm) | OD over (in) | OD over (mm) | OD under (in) | OD under (mm) |
|---|---|---|---|---|---|
| 1/8 –1-1/2, incl | [6–40], incl | 1/64 (0.015) | 0.4 | 1/32 (0.031) | 0.8 |
| Over 1-1/2 to 4, incl | Over [40 to 100] | 1/32 (0.031) | 0.8 | 1/32 (0.031) | 0.8 |
| Over 4 to 8, incl | Over [100 to 200] | 1/16 (0.062) | 1.6 | 1/32 (0.031) | 0.8 |
| Over 8 to 18, incl | Over [200 to 450] | 3/32 (0.093) | 2.4 | 1/32 (0.031) | 0.8 |
| Over 18 to 26, incl | Over [450 to 650] | 1/8 (0.125) | 3.2 | 1/32 (0.031) | 0.8 |
| Over 26 to 34, incl | Over [650 to 850] | 5/32 (0.156) | 4.0 | 1/32 (0.031) | 0.8 |
| Over 34 to 48, incl | Over [850 to 1200] | 3/16 (0.187) | 4.8 | 1/32 (0.031) | 0.8 |
Two features of this table matter in practice. First, the metric column is
not an independent number: every metric value is the inch value converted at
25.4 mm/in. and rounded to one decimal place, so a gauge reading 0.4 mm over
nominal on an NPS 1-1/2 duplex pipe is at the limit, not inside it. Second,
note the asymmetry in the first row: below NPS 1-1/2 the pipe may run 1/64 in.
(0.015) over nominal but 1/32 in. (0.031) under, so a small-diameter duplex
pipe 0.02 in. under nominal is still within tolerance. From NPS 1-1/2 to NPS 4
the band is symmetric at 1/32 in. (0.031) each way, and above NPS 4 the over
tolerance grows with size while the under tolerance stays fixed at 1/32 in.
(0.031).
For thin-wall pipe — defined in SA-999 12.2 as pipe whose wall
thickness is 3 % or less of the specified outside diameter — the Table 1
diameter tolerance applies only to the mean of the extreme maximum and minimum
outside diameter readings taken in any one cross-section, and the difference
between those extreme readings, meaning ovality, shall not exceed 1.5 % of the
specified outside diameter. SA-999 12.2 warns that thin-wall pipe usually
develops significant ovality during final annealing, straightening, or both, so
the Table 1 diameter tolerances on their own are usually not sufficient to
cover the ovality actually present in thin-wall duplex pipe.
2. Wall thickness tolerance — ASME SA-999 10.1
SA-999 10.1 sets the wall-thickness acceptance rule for both seamless and
welded pipe: the minimum wall thickness at any point shall not be more than
12.5 % under the nominal wall thickness specified. This is the single most
useful number on this page, because it converts the nominal schedule wall in
the dimension table above into the wall your ultrasonic gauge must actually
find. If your order calls for Sch 40S, the minimum wall anywhere on the pipe is
87.5 % of the nominal 40S wall, and anything thinner than that at any point is
a reject regardless of what the certificate says about the average.
SA-999 10.1.1 changes the picture entirely if the order specifies minimum
wall rather than nominal wall: in that case there shall be no variation under
the specified wall thickness, so the gauge must read at least the specified
figure everywhere on the pipe. SA-999 14.3 reinforces the distinction,
requiring the calculated mass per unit length to be determined from the nominal
wall thickness obtained from SA-999 Table X1.1 when minimum wall is specified in
the order.
The table below gives the minimum wall on inspection for each ANSI B36.19
schedule wall used in the dimension table above, so you can turn a schedule
number into a gauge reading without doing the arithmetic on site. Rows marked
SA-999 Table X1.1 are read directly from that printed table. Rows marked with
the NOTE 1 equation are calculated using the relationship ASME itself states
in NOTE 1 of Table X1.1, which is that the minimum wall equals the nominal
(average) wall multiplied by 0.875 — the same factor as the 12.5 % under
limit in 10.1, applied where the master table does not list that particular
nominal wall.
| Schedule | Nominal (average) wall, in. (mm) | Minimum wall on inspection, in. (mm) | Source |
|---|---|---|---|
| Sch 5S | 0.065 (1.7) | 0.057 (1.5) | SA-999 Table X1.1, NOTE 1 equation |
| Sch 5S | 0.109 (2.8) | 0.095 (2.4) | SA-999 Table X1.1, NOTE 1 equation |
| Sch 5S | 0.134 (3.4) | 0.117 (3.0) | SA-999 Table X1.1, NOTE 1 equation |
| Sch 5S | 0.160 (4.1) | 0.140 (3.6) | SA-999 Table X1.1, NOTE 1 equation |
| Sch 5S | 0.187 (4.7) | 0.164 (4.2) | SA-999 Table X1.1 |
| Sch 5S | 0.250 (6.3) | 0.219 (5.6) | SA-999 Table X1.1 |
| Sch 10S | 0.049 (1.2) | 0.043 (1.1) | SA-999 Table X1.1, NOTE 1 equation |
| Sch 10S | 0.065 (1.7) | 0.057 (1.5) | SA-999 Table X1.1, NOTE 1 equation |
| Sch 10S | 0.109 (2.8) | 0.095 (2.4) | SA-999 Table X1.1, NOTE 1 equation |
| Sch 10S | 0.134 (3.4) | 0.117 (3.0) | SA-999 Table X1.1, NOTE 1 equation |
| Sch 10S | 0.165 (4.2) | 0.144 (3.7) | SA-999 Table X1.1, NOTE 1 equation |
| Sch 10S | 0.188 (4.8) | 0.164 (4.2) | SA-999 Table X1.1 |
| Sch 10S | 0.250 (6.3) | 0.219 (5.6) | SA-999 Table X1.1 |
| Sch 40S | 0.068 (1.7) | 0.060 (1.5) | SA-999 Table X1.1 |
| Sch 40S | 0.088 (2.2) | 0.077 (1.9) | SA-999 Table X1.1, NOTE 1 equation |
| Sch 40S | 0.091 (2.3) | 0.080 (2.0) | SA-999 Table X1.1 |
| Sch 40S | 0.095 (2.4) | 0.083 (2.1) | SA-999 Table X1.1 |
| Sch 40S | 0.120 (3.0) | 0.105 (2.6) | SA-999 Table X1.1, NOTE 1 equation |
| Sch 40S | 0.133 (3.4) | 0.116 (2.9) | SA-999 Table X1.1 |
| Sch 40S | 0.180 (4.6) | 0.158 (4.0) | SA-999 Table X1.1, NOTE 1 equation |
| Sch 40S | 0.216 (5.5) | 0.189 (4.8) | SA-999 Table X1.1 |
| Sch 40S | 0.237 (6.0) | 0.207 (5.2) | SA-999 Table X1.1 |
| Sch 40S | 0.258 (6.6) | 0.226 (5.7) | SA-999 Table X1.1 |
| Sch 40S | 0.281 (7.1) | 0.246 (6.2) | SA-999 Table X1.1 |
| Sch 40S | 0.344 (8.7) | 0.301 (7.6) | SA-999 Table X1.1 |
| Sch 40S | 0.358 (9.1) | 0.313 (8.0) | SA-999 Table X1.1 |
| Sch 40S | 0.375 (9.5) | 0.328 (8.3) | SA-999 Table X1.1 |
| Sch 40S | 0.437 (11.1) | 0.382 (9.7) | SA-999 Table X1.1 |
| Sch 40S | 0.500 (12.7) | 0.438 (11.1) | SA-999 Table X1.1 |
| Sch 40S | 0.531 (13.5) | 0.465 (11.8) | SA-999 Table X1.1 |
| Sch 40S | 0.562 (14.3) | 0.492 (12.5) | SA-999 Table X1.1 |
| Sch 40S | 0.594 (15.1) | 0.520 (13.2) | SA-999 Table X1.1, NOTE 1 equation |
| Sch 40S | 0.625 (15.9) | 0.547 (13.9) | SA-999 Table X1.1 |
| Sch 40S | 0.719 (18.3) | 0.629 (16.0) | SA-999 Table X1.1 |
| Sch 40S | 0.812 (20.6) | 0.710 (18.0) | SA-999 Table X1.1 |
| Sch 40S | 0.906 (23.0) | 0.793 (20.1) | SA-999 Table X1.1, NOTE 1 equation |
| Sch 40S | 1.000 (25.4) | 0.875 (22.2) | SA-999 Table X1.1 |
| Sch 40S | 1.125 (28.6) | 0.984 (25.0) | SA-999 Table X1.1 |
| Sch 40S | 1.250 (31.8) | 1.094 (27.8) | SA-999 Table X1.1 |
| Sch 40S | 1.375 (34.9) | 1.203 (30.6) | SA-999 Table X1.1 |
| Sch 40S | 1.500 (38.1) | 1.312 (33.3) | SA-999 Table X1.1, NOTE 1 equation |
| Sch 80S | 0.095 (2.4) | 0.083 (2.1) | SA-999 Table X1.1 |
| Sch 80S | 0.119 (3.0) | 0.104 (2.6) | SA-999 Table X1.1 |
| Sch 80S | 0.126 (3.2) | 0.110 (2.8) | SA-999 Table X1.1 |
| Sch 80S | 0.147 (3.7) | 0.129 (3.3) | SA-999 Table X1.1 |
| Sch 80S | 0.188 (4.8) | 0.164 (4.2) | SA-999 Table X1.1 |
| Sch 80S | 0.203 (5.2) | 0.178 (4.5) | SA-999 Table X1.1 |
| Sch 80S | 0.237 (6.0) | 0.207 (5.2) | SA-999 Table X1.1 |
| Sch 80S | 0.281 (7.1) | 0.246 (6.2) | SA-999 Table X1.1 |
| Sch 80S | 0.344 (8.7) | 0.301 (7.6) | SA-999 Table X1.1 |
| Sch 80S | 0.375 (9.5) | 0.328 (8.3) | SA-999 Table X1.1 |
| Sch 80S | 0.469 (11.9) | 0.410 (10.4) | SA-999 Table X1.1, NOTE 1 equation |
| Sch 80S | 0.500 (12.7) | 0.438 (11.1) | SA-999 Table X1.1 |
| Sch 80S | 0.594 (15.1) | 0.520 (13.2) | SA-999 Table X1.1, NOTE 1 equation |
| Sch 80S | 0.719 (18.3) | 0.629 (16.0) | SA-999 Table X1.1 |
| Sch 80S | 0.812 (20.6) | 0.710 (18.0) | SA-999 Table X1.1 |
| Sch 80S | 0.938 (23.8) | 0.821 (20.8) | SA-999 Table X1.1, NOTE 1 equation |
| Sch 80S | 1.125 (28.6) | 0.984 (25.0) | SA-999 Table X1.1 |
| Sch 80S | 1.312 (33.3) | 1.148 (29.2) | SA-999 Table X1.1 |
| Sch 80S | 1.500 (38.1) | 1.312 (33.3) | SA-999 Table X1.1, NOTE 1 equation |
| Sch 80S | 1.750 (44.4) | 1.531 (38.9) | SA-999 Table X1.1 |
One practical consequence is worth stating plainly. The wall you order is
the nominal figure, and 12.5 % is the margin the mill is permitted to work in
below it. When you compare delivered pipe against the schedule you specified,
ask for the wall thickness actually measured at the weld seam in the mill
certificate, because that is the figure the 12.5 % rule is applied to. A
certificate quoting a nominal wall tells you nothing about the thinnest point
on the pipe.
3. Length, straightness and mass
Straightness on seamless pipe follows SA-999 16.1, which requires only that the finished pipe be reasonably straight. The numeric 1/8 in. (3.2 mm) deviation over a 10 ft (3.0 m) straightedge in SA-999 16.2 is written for metal-arc welded pipe, so it is quoted on our welded grade rather than on this seamless grade. On length, SA-999 13.1 governs definite cut lengths of 24 ft
(7.3 m) or less for both seamless and welded pipe: no length shall be under
the length specified, nor more than 1/4 in. (6 mm) over it, with lengths
greater than 24 ft (7.3 m) subject to agreement between manufacturer and
purchaser. On mass, SA-999 9.1 states that the mass of any length of seamless
pipe in sizes NPS 12 and smaller shall not vary more than 10 % over or more
than 3.5 % under the specified mass; for pipe larger than NPS 12 the band is
10 % over and 5 % under. Where minimum wall is specified in the order, SA-999
9.2 widens the mass band to 16 % over the mass calculated per 14.3.
For a seamless duplex order the acceptance sequence is therefore: check the
outside diameter against SA-999 Table 1 for that size band, check the minimum
wall against SA-999 10.1 at the weld seam and at the mid-length, check the
length against SA-999 13.1, and check the stated mass against SA-999 9.1. All
four checks come from one document, so a certificate that quotes them is
internally consistent, and a certificate that quotes none of them is telling
you that the mill has not measured against the standard that governs its own
product. SA-789, SA-790 and SA-312 compared sets out the other
specifications a duplex order normally has to name.
Frequently Asked Questions
Which ASME specification covers duplex 2205 seamless pipe?
ASME SA-790, identical to ASTM A790/A790M, Seamless and Welded Ferritic/Austenitic
Stainless Steel Pipe. SA-789 is the tubing specification for the same alloys, and
SA-182 covers forged flanges, fittings and valves. Quote the form you need.
Is SA-790 the right specification, or should I ask for SA-789?
SA-790 for pipe, SA-789 for tube. They carry the same UNS numbers and largely the
same chemistry, but they are different documents with different scope, dimensional and
inspection requirements, so a certificate written to one is not automatically
compliant with the other.
What is the difference between S32205 and S31803?
S32205 is the tightened-nitrogen version: chromium 22.0–23.0 %, molybdenum
3.0–3.5 %, nitrogen 0.14–0.20 %. S31803 is the earlier, wider window at
chromium 21.0–23.0 %, molybdenum 2.5–3.5 %, nitrogen 0.08–0.20 %. S32205
also carries the higher tensile minimum of 95 ksi (655 MPa) against 90 ksi (620 MPa),
with the same 65 ksi (450 MPa) yield in both.
Is impact testing required?
Not by the base specifications for this grade. SA-182 9.7 applies the notch
toughness requirement to F 3V, F 3VCb and F 22V, and SA-790 does not impose a Charpy
requirement on S32205. If your project calls for impact testing or a corrosion test,
state it on the order as a supplementary requirement and we will run it.
What certification is supplied?
EN 10204 3.1 mill test certificate as standard, including the heat treatment
condition, product analysis, tensile and hardness results. EN 10204 3.2 is issued when
third-party inspection is specified on the purchase order.
Can this pipe be threaded?
Not on the 5S or 10S schedules. SA-790 Table X1.1 note A states that schedules 5S
and 10S wall thicknesses do not permit threading in accordance with ANSI B1.20.1.
Schedule 40S and 80S walls are the threadable schedules in the B36.19 series.
For the wider context of how a duplex grade fits alongside the nickel alloy seamless pipe and tube families, our the wider nickel alloy seamless pipe and tube range page sets out the grades and product forms we supply.
What should I check before ordering Duplex 2205 Seamless Pipe?
What specifications cover Duplex 2205 Seamless Pipe?
Duplex 2205 Seamless Pipe is supplied to ASME SA-790, ASTM A790, ASME SA-789, as detailed in the specification sections on this page. Equivalent EN, AMS or GB standards can be discussed on request.
What certification is supplied with Duplex 2205 Seamless Pipe?
Every lot is delivered with an EN 10204 3.1 mill test certificate covering the heat number and the inspection results for that lot.
What size range can I order for seamless pipe and tube?
Nickel alloy seamless pipe is listed as OD 6-610 mm with wall thickness 0.5-40 mm. For duplex and stainless grades, send the required OD, wall and schedule and we will confirm the available range against the ordered ASTM / ASME specification. The size and schedule tables are in our seamless pipe and tube guide.
How do I request a quote for Duplex 2205 Seamless Pipe?
Email info@nickelalloyseamlesspipe.com or WhatsApp +86 186 2137 7760 with your grade, size and quantity. Our engineers reply within 8 working hours.