Filler Metal Selection for Stainless and Nickel Alloy Pipe

ASME Section II fixes the filler metal, the preheat and interpass range and the post-weld heat treatment for every grade. This article shows where those numbers live and how to write them into a purchase order.

Welding a nickel alloy pipe is not a procedure you invent on the fabrication floor. The filler metal, the heat input range and the post-weld heat treatment are fixed in advance by the material specification, and a buyer who knows where those numbers live can put them on the purchase order rather than discovering them later.

This article works through the welding clauses that matter for stainless steel and nickel alloy pipe, taken from the ASME BPVC 2023 Section II material volume: SA-312, SA-182, SA-961, SA-999 and SA-333.

Two different welding problems: making the pipe, and fixing the pipe

For the manufacturing weld, SA-312 §6.1.3 is blunt: welded (WLD) pipe shall be made using an automatic welding process with no addition of filler metal during the welding process. §6.1.4 makes the same statement for heavily cold-worked (HCW) pipe and requires the weld to be 100 % radiographically inspected per Paragraph UW-51 of Section VIII, Division 1 before cold working. SA-789/SA-789M §5.1 is equivalent for tubing.

Repair welding is the opposite case. SA-312 §15.3 requires weld repairs to be made only with the gas tungsten-arc process, using the same classification of bare filler rod qualified to the most current AWS Specification A5.9 as the grade being repaired, and as shown in Table 6 of SA-312 itself. Alternatively, and only with purchaser approval, a filler metal more highly alloyed than the base metal may be used where needed for corrosion resistance.

The filler table in SA-312 Table 6

SA-312 Table 6, “Pipe and Filler Metal Specification”, maps each pipe grade to the filler class a repair weld must use, nickel alloy grades included.

Pipe gradeUNSFiller classFiller metal UNS
TP304S30400ER308S30800, W30840
TP304LS30403ER308LS30883, W30843
TP316S31600ER316S31680, W31640
TP316LS31603ER316LS31683, W31643
TP321S32100ER321 or ER347S32180, W32140 or S34780, W34740
Alloy 20N08020ER320 or ER320LRN08021 or N08022
Alloy 29N08029ERNiCrMo-3A or ERNiCrMo-13AN06625 or N06059
800 / 800HN08800 / N08810ERNiCr-3AN06082

Two details matter. The table carries two filler specifications, and the stainless and nickel alloy grades fall in different ones: the 800 and 800H rows specify ERNiCr-3A, UNS N06082, a nickel alloy filler, so an Alloy 800 repair is not a stainless repair. Second, the table names no filler classification for every grade — for N08367, N08925 and N08926 the filler metal UNS listed is N06625 while the classification cell is blank, deferring the choice to the parties.

For nickel alloy forgings, SA-182 §15.1.2 gives the equivalent mapping: the weld metal shall correspond either to the base metal alloy content or to a named AWS classification — E209/ER209 for S20910; ENiCrMo-3, -4 or -10 and their ER equivalents for N08367, N08700, N08925 and N08926; E320/E320LR or ER320/320LR for N08020; ENiCr-3/ERNiCr-3 for N08800, N08810 and N08811.

Dissimilar joints: where the weld chemistry has to be calculated

SA-182 §15.1.2.1 governs welding a nickel alloy to something else. For weld deposits on S20910, N08020, N08367, N08700, N08800, N08810, N08811, N08925 and N08926, the filler metal shall have a composition conforming to the base material or the equivalent AWS A5.11 and A5.14 classification. The weld deposit chemistry shall meet the lowest minimum and highest maximum values for each element in either the base metal or filler metal specification. Dilution must be considered for over-alloyed fillers, and the deposit chemistry tested and recorded on the Procedure Qualification Record.

That is a computational requirement, not a formality. A welder running a nickel alloy pipe against a stainless flange qualifies the deposit against the intersection of two chemistry envelopes, and the lower of the two minimums and the higher of the two maximums govern.

Heat input: what the specification actually permits

SA-182 Table 4, “Repair Welding Requirements”, sets preheat, interpass temperature and post-weld heat treatment, grade by grade.

GradeElectrodesPreheat and interpass, °F [°C]Post-weld heat treatment, °F [°C]
F 304 / F 316E 308 / E 316, -15 or -16NR1900 [1040] + WQ
F 304L / F 316LE 308L / E 316L, -15 or -16NR1900 [1040] + WQ
F 347 / F 347HE 347-15 or 16 / -16HNR1900 [1040] / 1925 [1050] + WQ
F 51 (duplex)—NRNR
F 53, F 55, F 60 (super duplex / duplex)—NRNR
F 20 (Alloy 20)E/ER-320, 320LRNR1700–1850 [925–1010] + WQ
F 44 (6% Mo)E NiCrMo-3NR2100 [1150] + WQ
F 62 (6XN)E NiCrMo-3NR2025 [1105] + WQ
F 70 (Alloy 800)ERNiCr-3, ERNiCrMo-3 or ERNiCrMo-4NR1900 [1040] + WQ
F 904LE NiCrMo-3NR1920–2100 [1050–1150] + WQ

“NR” means not required, “WQ” means water quench. Every austenitic stainless grade carries no preheat and no interpass limit, because austenitic stainless does not need one; the grades carrying a specific post-weld heat treatment do so because that treatment restores corrosion resistance after the weld has been through the hot zone. The duplex rows are NR on both counts, consistent with SA-182 Table 1 requiring a full solution treatment.

The nickel alloy entries differ from each other. F 70 takes ERNiCr-3, ERNiCrMo-3 or ERNiCrMo-4 as a choice of three; F 62 takes only E NiCrMo-3 with a PWHT of 2025 [1105] + WQ; F 904L takes E NiCrMo-3 with a PWHT range rather than a single figure.

When repair welding is allowed at all

SA-182 §15.1.6 states that repair by welding shall not exceed 10 % of the surface area of the forging, nor 33⅓ % of the wall thickness, nor 3/8 in. [9.5 mm], whichever is less, without prior purchaser approval. §15.1.5 allows austenitic stainless forgings to be repair-welded without the Table 4 post-weld heat treatment, with prior approval. §15.1.8 is categorical: no weld repairs are permitted for F 6a Classes 3 and 4.

On the pipe side, SA-312 §15.2 limits seam repairs to 20 % of the seam length, and §15.4 requires that pipes with seam repairs be uniquely identified on the certificate of tests, with the filler metal identified when it is not the Table 6 filler. SA-999 §17.1 adds the point that matters most to a buyer: repair by welding is permitted subject to purchaser approval, and the deposited filler metal shall be suitable for the composition being welded. Each repaired length shall then be reheat treated or stress relieved as the product specification requires, and nondestructively tested.

For low-temperature service the rule is tighter still. SA-333 §4.2.3 requires all welded joints to be fully radiographed per Paragraph UW-51 of Section VIII, Division 1, with ultrasonic examination under Appendix 12 as the alternative. §4.2.4.2 requires each repair weld of a cavity whose depth before repair exceeds the lesser of 3/8 in. [9.5 mm] or 10.5 % of nominal thickness to be radiographically examined as the original welds are.

Qualification, marking, and what to put on the order

All of the above assumes qualified welders. SA-961 §16.1.1 requires the welding procedure and welders to be qualified in accordance with Section IX of the ASME Boiler and Pressure Vessel Code, and SA-999 §17.2 requires repair welding to use procedures and welders qualified to Section IX as well. Supplementary Requirement S58.1 to SA-961 is shorter and more absolute: no repair welding shall be permitted without prior purchaser approval.

The marking tells the story. SA-182 §19.1.2 requires forgings repaired by welding to be marked with the letter “W” after the specification designation, and where a repair-welded austenitic stainless forging has not been postweld heat treated per Table 4, the letters “WNS” shall be marked. SA-999 §26.4 requires pipes weld repaired per §17.1 to be marked “WR”. A W or WR mark means the component was welded after manufacture; WNS means welded without PWHT.

Four items decide the answer for a pipe enquiry involving welding, and all are free to specify in advance: the grade and product form, which fix the filler class, preheat and post-weld heat treatment; whether repair welding is permitted and whether it needs prior approval; the dissimilar-joint rule; and which specification governs the repair — SA-312 §15 for pipe, SA-182 §15 for forgings, SA-333 §4.2 for cold service, SA-999 §17 generally, SA-961 §16 for stainless forgings.

One more point, because it catches people out. SA-182 has no F 625 and no F C-276 grade, so a quotation against SA-182 for a 625 or C-276 forging quotes a grade that does not exist. Forged Alloy 625 and C-276 components are governed by SB-564, and the flanges and fittings by SB-462, whose scope lists N10276 but not N06625.

If you have a welding package to price and the grade is not settled, send us the grade, the product form and the joint configuration, and we will confirm the filler class, the heat input range and the repair limits the specifications allow. Reach us on WhatsApp at +86 186 2137 7760 or through our contact page, and ask about our 316 and 316L seamless pipe when corrosion decides the case.

Related products: nickel alloy seamless pipe and tube · Inconel 625 seamless pipe · Hastelloy C-276 seamless pipe · pipe and tube. Supplied to the applicable ASTM / ASME specifications with EN 10204 3.1 mill test certificates; confirm grade, size and quantity with our engineers.

Product Enquiry