For UNS N06625, the word grade does not mean what it means for most other alloys. It is not a composition grade. It is a heat treatment condition, and the specification supplies it for you if your order does not. Both SB-444 and SB-443 say the same thing in the same words: if neither grade of N06625 is specified, Grade 1 will be supplied.
That default is reasonable at ordinary temperatures and actively wrong at high ones, because the grade that is stronger is the grade that is not for hot service. What follows is how the four nickel alloy pipe and plate specifications divide service temperature, and why the strength numbers move the way they do.
Grade 1 is stronger, and that is why it is the wrong grade above 1100 F
SB-444 Section 1.1.1 sets the split. Grade 1, annealed, is normally employed in service temperatures up to 1100 F (593 C). Grade 2, solution annealed, is normally employed in service temperatures above 1100 F when resistance to creep and rupture is required. The strength table for the same alloy, in the same specification, then reads in the opposite direction to intuition.
| SB-444 Table 1, UNS N06625 | Tensile min, ksi (MPa) | Yield min, ksi (MPa) | Elongation in 2 in. min, % |
|---|---|---|---|
| Grade 1, annealed (1600 F / 871 C minimum) | 120 (827) | 60 (414) | 30 |
| Grade 2, solution annealed (2000 F / 1093 C minimum) | 100 (690) | 40 (276) | 30 |
| N06852, solution annealed | 85 (586) | 35 (241) | 30 |
| N06219, solution annealed | 96 (660) | 39 (270) | 30 |
So the grade with 20 percent more tensile strength is the one whose service ceiling is 1100 F, and the grade with the lower strength is the one specified for temperatures above it, where the material has to hold against creep and rupture rather than against a static load. The explanation is the heat treatment, and it is in the same table. Grade 1 is annealed, which leaves chromium and columbium carbides at the grain boundaries. Grade 2 is solution annealed at 2000 F, with or without a subsequent stabilization anneal at 1800 F minimum, and that treatment is what delivers the full chromium, molybdenum and columbium solid solution without the grain boundary precipitation that annealing leaves behind.
The same 1100 F line runs through four specifications
What makes this a convention rather than a coincidence is that the alloy family divides on the same boundary everywhere it appears. Four specifications make the same assignment, and a buyer who moves between them needs to notice it.
| Specification | Product form | Grade normally used up to and including 1100 F (593 C) | Grade normally used above 1100 F, where creep and rupture resistance is required |
|---|---|---|---|
| SB-407 | Cold-worked and hot-finished annealed seamless pipe and tube | N08800 and N06811 | N08120, N08810, N08811 and N08890, annealed to develop controlled grain size for optimum properties in this range |
| SB-443 | Rolled plate, sheet and strip | Grade 1, annealed | Grade 2, solution annealed |
| SB-444 | Cold-worked seamless pipe and tube | Grade 1, annealed | Grade 2, solution annealed |
| SB-564 | Forgings | N08800 | N08810, N08120 and N08811, annealed to develop controlled grain size for optimum properties in this range |
Note what the last two rows say together. For a 625 pipe, the specification calls for Grade 2 above 1100 F because creep governs. For an 800H forging, the specification does not name a grade at all. It names a condition and a grain size, because grain boundary condition is what controls creep resistance in that family.
And Grade 1 itself means different strengths in different product forms
Even within one grade designation, the plate specification does not give one number. SB-443 Table 3 separates Grade 1 by how the material was rolled, because cold working raises strength and the specification reflects that in the minimum.
| SB-443 Table 3, UNS N06625 Grade 1, annealed | Tensile min, ksi (MPa) | Yield min, ksi (MPa) | Elongation in 2 in. min, % |
|---|---|---|---|
| Cold-rolled sheet and strip | 120 (827) | 60 (414) | 30 |
| Hot-rolled sheet and hot-rolled plate up to 2.75 in. (70 mm) incl. | 110 (758) | 55 (379) | 30 |
| Cold-rolled plate up to 0.375 in. (9.5 mm) incl. | 110 (758) | 55 (379) | 30 |
| Grade 2, solution annealed, all forms | 100 (690) | 40 (276) | 30 |
The footnote to that table closes the two small-material loopholes in the ordinary way: yield strength requirements do not apply to material under 0.020 in. (0.508 mm) thick, and elongation requirements do not apply to material under 0.010 in. (0.254 mm) thick. So the material form, the thickness and the rolling route each decide which number you are actually held to.
Two more provisions in SB-444 deserve attention before an order is placed. Section 1.1 carries a note stating that hot working or reannealing may change properties significantly, depending on working history and temperatures, which matters if a mill is buying in annealed stock and forming it after the fact. And Section 9.1 sets the allowable fibre stress for the hydrostatic test by grade: 30,000 psi (207 MPa) for Grade 1, 25,000 psi (172 MPa) for Grade 2, 24,000 psi (165 MPa) for N06219 and 21,000 psi (145 MPa) for N06852, with 1.5 times those values available only when the manufacturer and the purchaser agree.
What to put on the order
- Name the grade. Grade 1 or Grade 2, explicitly. Silence gets you Grade 1 in both SB-443 and SB-444.
- Name the product form as well: sheet and strip in coil, cut straight lengths or random straight lengths, how plate is to be cut, and thickness, width and length, per SB-443 Section 4.1.5 to 4.1.7.2.
- Name the finish. SB-444 Appendix X2 lists the conditions normally supplied: cold-drawn, annealed or solution annealed with ground outside diameter in sizes from 1/2 to 4 in. (12.7 to 102 mm), or cold-drawn, annealed or solution annealed and pickled, not ground, in sizes from 1/2 to 6-5/8 in. (12.7 to 168 mm). The same appendix lists the converter sizes, small-diameter and light-wall tube in outside diameters of 1-1/4 in. (31.8 mm) and under, for which the manufacturer should be consulted on which sizes and wall thicknesses can be furnished.
- Name the test. Section 9.1 requires the hydrostatic test at the grade allowable fibre stress, Section 9.2 requires nondestructive electric examination, and the order has to say which route applies.
- Say whether you want a product check analysis and whether you will witness inspection. Both are optional requirements in the order information list, and Section 4.1.10 requires the order to state which tests or inspections are to be witnessed if the purchaser wants that.
We supply our Incoloy 800 and 800H seamless pipe and the Inconel 625 pipe and tube product page, along with our nickel alloy plate and sheet, and we can quote any of the grades and conditions above with the certificate and the marking to suit your contract. If you want a written recommendation for a service temperature rather than a price, request an Alloy 625 pipe quotation and tell us the design temperature, whether the material will be formed after delivery, and which specification and edition your client has named.